How to repair a stripped thread with Belzona 1111

In this video, Rezitech’s Belzona Technical & Training Manager, Charlie Farrant, shows how to rebuild a stripped or damaged thread using Belzona 1111 Super Metal. The demonstration uses a bearing end cap from a liquid ring vacuum pump with a scored, damaged thread.

The repair uses the original bolt as a mould. Belzona 9411 release agent is applied first, so the Belzona 1111 forms around the bolt without sticking to it. The video takes you through each stage: grinding the damaged thread to an angular profile, mixing Belzona 1111, filling the prepared hole, and screwing in the coated bolt to form a new thread.

This method is a quick, cost-effective way to restore stripped or damaged threads without replacing the component. It can be done in the workshop or on site.

Charlie Farrant Rezitech Belzona Technical & Training Manager

Charlie Farrant 

Belzona Technical & Training Manager

Step-by-step guide

This guide follows the Rezitech Services demo with Charlie. He rebuilds the scored thread in a bearing end cap from a liquid ring vacuum pump, using the bolt as a mould for the new thread.

Step 1: Apply Belzona 9411 release agent to the bolts (0:39–1:13)

  • The bolts are used to form the new thread, so Belzona must not stick to them. Belzona 9411 release agent stops that.
  • Apply two thin coats to the bolt threads.
  • Let the first coat dry for about 35–40 minutes before applying the second coat.
  • After the second coat, allow another 35–40 minutes before using the bolts.
  • Tip: Do this at the very start of the job so the bolts are drying while you prepare the surface.

Step 2: Prepare the surface to create an angular profile (1:25–2:35)

  • Surface preparation is the most important part of any Belzona application.
  • Drill out the damaged thread (1:36). Use a drill bit one size bigger than the bolt to remove the scored, damaged thread.
  • Profile the hole with a die grinder (1:46). This gives the surface a rough, angular profile so Belzona 1111 can grip it mechanically.
  • Clean the repair area (5:09). After grinding, clean the area with ReziSafe FP29 solvent to remove dust, oil and other contamination.
  • Seal the back of the hole (7:40). Block off the back of the hole so the material can’t squeeze out too far when the bolt goes in.

Step 3: Measure out Belzona 1111 (2:35–2:48)

  • Measure 3 parts base to 1 part solidifier by volume.
  • Mix only as much as the repair needs. This is a small repair, so only a small amount is used.

Step 4: Mix Belzona 1111 (2:48–4:54)

  • Start mixing (2:48). Pull the two components into a mound in the middle of the Belzona mixing board.
  • Mix in a figure-of-eight motion (3:02). Press down firmly on the spatula, using your thumb on the edge of the blade.
  • Scrape and turn (3:14). Scrape the material up with the serrated edge of the spatula, then turn the board around rather than using the back of the spatula. Repeat the figure-of-eight mixing.
  • Clean the spatula edge (3:49). Wipe the spatula edge to remove unmixed material, then do a strike-through to check the mix.
  • Mix once more (4:15). Give it one extra pass for good measure, even if it already looks good.
  • Spread it thin (4:28). Spread the mixed material thinly across the board so it lasts longer before it cures.
  • Check the colour (4:44). The mix is ready when it is one consistent colour, with no streaks or marbling.

Step 5: Apply Belzona 1111 and form the thread (4:54–8:34)

  • Run a pre-application check (4:54). Confirm the surface has been ground and cleaned, the bolts are released and cured, and the material is mixed.
  • Brush on the first layer (5:25). Use a brush with the bristles cut short and gently work Belzona into the threaded area for a good imprint.
  • Work it into the profile (6:35). This first layer is critical, because it pushes into the angular profile and gives maximum adhesion.
  • Build up the material (7:01). Once the surface is fully wetted out, keep feeding material into the hole with the brush or spatula until it is completely filled. A small amount will start to squeeze out.
  • Insert the bolt (7:48). Push the released bolt into the hole while twisting it clockwise, and drive it all the way in.
  • Tidy up the excess (8:14). Remove the worst of the excess material now. Final clean-up can be done by sanding once the material has cured.

Step 6: Cure, remove the bolt and inspect the thread (8:34–9:31)

  • Leave it to cure (8:34–8:55). Allow about 2–3 hours at 20–25°C before removing the bolt.
  • Crack the bolt free (9:02). Use a spanner to break the bolt free, back it out partway, then finish removing it by hand.
  • Inspect the result (9:23). The bolt should come out clean, with no Belzona stuck to it, leaving a newly formed thread in the component.
Belzona 1111

Any Questions?

Fill out the form below and we’ll get back to you as soon as possible.

Frequently asked questions

Yes. You can rebuild a stripped, scored or damaged internal thread with Belzona 1111 Super Metal, using the original bolt as a mould. First, drill out the damaged thread one size larger than the bolt and grind the hole to an angular profile. Next, fill the hole with Belzona 1111. Then screw in a bolt coated with release agent and leave it to cure. When the bolt is removed, a new, fully formed thread is left behind. Rezitech Services uses this method on pump components such as liquid ring vacuum pump bearing end caps.

Coat the bolt with Belzona 9411 release agent before you use it. Apply two thin coats, allowing 35–40 minutes of drying time after each one. That adds up to about 70–80 minutes before the bolt is ready. Apply the release agent at the start of the job so the bolts are drying while you prepare the repair surface. Once the Belzona has cured, the bolt unscrews cleanly with no material stuck to its threads.

Surface preparation is the most important step in any Belzona repair. It involves four steps:

  • Drill out the damaged thread with a drill bit one size larger than the bolt.
  • Use a die grinder to create a rough, angular profile inside the hole, which gives the strongest mechanical bond.
  • Clean the area with a solvent such as ReziSafe FP29.
  • Block off the back of the hole so the material can’t squeeze through.

Belzona 1111 Super Metal is mixed at 3 parts base to 1 part solidifier by volume. Mix it on a Belzona mixing board with a spatula, using a firm figure-of-eight motion. Scrape the material up regularly and turn the board around as you go. Clean any unmixed material off the spatula edge, then do a strike-through to check the mix. It is fully mixed when it is one consistent colour, with no streaks or marbling. Spread the mixed material thinly on the board so it stays workable for longer.

In the Rezitech demonstration, Belzona 1111 was left to cure for about 2–3 hours at 20–25°C before the bolt was removed. Break the bolt free with a spanner, then unscrew it the rest of the way by hand. The rebuilt thread is left in the component. Cure times are longer at lower temperatures, so check the Belzona product data sheet for your conditions before putting the part back into service.